Do you feel the printed silicone transfer logo is not enough matte or skin touch feeling after printing matte silicone?
There are three reasons may caused this matte problem.
First, Choosing the best matte film. Our FY silicone can supply you the best matte film which is the most matte one for silicone transfer printing in the market.
Second, before the last step to print matte silicone, we can print 2 layers with glossy silicone and pigment firstly to increase matte and skin touch feeling.
Third, please try to use the best quality matte silicone which is super matte.

How to skin feel super matte forward silicone heat transfer?
Preparation before forward silicone heat transfer printing:
Silicone ink PET films: Matte film
Mesh number: 120-200 (48-80T) , Mesh(screen film )thickness 0.1-0.2MM,it is depends on printing Artworks.
Squeegee:65-80 degree
orward silicone transfer printing process with skin feel super matte effect:
1 Hot melt glue FY-HP-01G print for 8 layers.
Hot melt glue FY-HP-01G 50G
Thinner FY-5# 10-15G 20-30%
Flash by room temp or by 80-100 degree.
To mix 20-30% hot melt glue thinner FY-5# to dilute the glue to avoid choking the mesh when printing. If mix with more glue thinner then need print more layers. The glue thinner can be also used to wash the mesh after glue printing.
2 Transfer crossing linker 2 layers :
Silicone crossing linker FY-2900A 50G
Silicone crossing linker catalyst FY-2900B 5G 10%
Flash by 100 degree.
TIPS: The effective printing time after mixing with agent FY-2900B is more than 1 hour not reach 2 hours, so please reasonably mix crossing linker and crossing linker curing agent to avoid waste.
3 Clear printing 2-16 layers for high density
HD Transfer silicone FY-1320 100G
Silicone thinner FY-1# 10-20G 10-20%
Silicone catalyst FY-003 10G 10% Flash by 100 to120 degree.
4 Transfer silicone color printing for 5 layers
Round Transfer silicone FY-3030 100G
Silicone thinner FY-1# 10-20G 10-20%
Silicone pigments 20G 20%
Silicone catalyst FY-003 10G 10%
Flash by 100 to120 degree.
5 Print 2 layers with glossy silicone and pigment
Glossy silicone FY-1025 100G
Silicone thinner FY-1# 10-20G 10-20%
Silicone pigments 10-20G 10-20%
Silicone catalyst FY-003 10G 10%
6 Print 3 layers with round silicone and pigment using another mesh
Round Transfer silicone FY-3030 100G
Silicone thinner FY-1# 10-20G 10-20%
Silicone pigments 20G 20%
Silicone catalyst FY-003 10G 10%
7 Print matte silicone ink with 1 layer for top coating
Matte silicone FY-1000M 50G
Slow dry catalyst FY-003 5G 10%
8 After finish, put into the oven to bake by 100 degrees for 30 minutes.
9 Heat press the film on the fabric by the temp of 160 degrees for both sides 10-15 seconds.



If you are encountering this problem, please contact Ola from FY silicone, Whatsapp +8613423132667. Let me show you how to resolve this problem.